| Vicrosity, KU | ||
| Initial | Kreb Units | 123 |
| Heat Aged | Kreb Units | 126 |
| |
||
| pH | ||
| Initial | Unstated | 8.9 |
| Heat Aged | Unstated | 8.5 |
| Adhesion - Dry (PLI) | ||
| Mod. Bitumen | ASTM C794 | 0.8 A |
| Concrete Block | ASTM C794 | 8.9 A, C |
| Galvanized | ASTM C794 | 2.2 A |
| Asphalt Shingle | ASTM C794 | 2.0 A, C |
| Adhesion - Wet (PLI) | ||
| Mod. Bitumen | ASTM C794 | 0.5 A |
| Concrete Block | ASTM C794 | 14.2 C, CP |
| Galvanized | ASTM C794 | 1.9 A |
| Asphalt Shingle | ASTM C794 | 0.6 AC |
| Early Blister Resistance | ||
| 16 Hour Cure | Unstated | NO BLISTERS |
| 24 Hour, water 25mil | Unstated | NO BLISTERS |
| Salt Spray Resistance | ||
| 11 Days Salt Spray | ASTM B117, ASTM D1654 | 10 |
| Water Swelling % | ||
| 24 Hour Immersion | ASTM D823, ASTM D471 | 16.9% |
| PERMS | ASTM D1653, ASTM E 96 | 5 |
| 50 Hours W-O-M Elongation | ||
| Room Temperature | ||
| % to max. Stress | ASTM D412 | 700% |
| % to Break | ASTM D412 | 700% |
| % Recovery | ASTM D412 | 44% |
| 32 Degrees F. | ||
| % to max. Stress | ASTM D412 | 430% |
| % to Break | ASTM D412 | 430% |
| % Recovery | ASTM D412 | 28% |
| Tensile Strength, PSI | ||
| Room Temperature | ||
| % to max. Stress | ASTM D2370 | 1350 PSI |
| % to Break | ASTM D2370 | 1350 PSI |